Fabric Composition Testing: How a Lab Proves 65/35, and Why It Varies
Fabric composition test explained: how labs dissolve one fibre to prove a blend ratio, why moisture, finish and sampling shift results, and how to word it.

A fabric composition test proves a blend ratio by chemistry, not by eye. The lab dissolves one fibre with a selective reagent, weighs the dried residue and calculates each share by mass. For polyester-cotton, 75% sulphuric acid removes the cotton. Specify the method, the reporting basis and an agreed tolerance, because those choices move the number.
How does a fabric composition test prove a blend ratio?
Quantitative fibre analysis is a mass balance: identify the fibres, clean and dry a specimen, dissolve one fibre, then weigh what survives.
If a specimen has a dry mass of 1.000 g and the polyester residue has a dry mass of 0.652 g, the result is 0.652 ÷ 1.000 × 100 = 65.2% polyester. The other 34.8% is found by difference, not measured directly. These figures are illustrative, but the logic explains many disputes: anything that disappears with the dissolved fibre gets counted as that fibre.
A ratio describes the whole fabric, not the yarn name on the spec. Take a 65/35 polyester-cotton warp with a 100% cotton weft, and assume the warp makes up 60% of the fabric's mass. Polyester is 0.60 × 65 = 39%, so the fabric tests near 39/61, whatever the warp yarn is called. State fabric and yarn composition separately. For the performance side of the decision, see how to choose a poly-cotton ratio.
Which test method is used for polyester-cotton blends?
The usual ISO route is ISO 1833-11:2017, the sulphuric acid method for mixtures of certain cellulose fibres with certain other fibres, polyester among them. ISO 1833-1:2020 sets the general principles for the series, and fibre identification comes first: the matching method in EU Regulation 1007/2011 requires it outright. AATCC publishes a separate quantitative method, so name one method rather than writing "lab tested".
| Tool | What it tells you | Can it prove 65/35? | Use it for |
|---|---|---|---|
| Burn test | Cellulose chars to soft ash; polyester melts into a hard bead | No | Quick check that a synthetic is present |
| Microscopy | Fibre types present, from their appearance | No, treat as screening here | Identifying fibres before the chemical test |
| Sulphuric acid dissolution (ISO 1833-11) | Polyester share by residue mass; cellulose by difference | Yes, for fibres in its scope | Polyester-cotton claims on a contract |
The acid dissolves cellulose as a group, and the scope covers viscose, modal and lyocell as well as cotton. A cotton-viscose-polyester cloth therefore does not get a cotton figure from this step alone. Elastane is not among the fibres listed in the part's scope, so ask the lab which route it would use for a stretch blend. And a dissolution test cannot separate recycled polyester from virgin polyester, or organic cotton from conventional, because the fibre chemistry is the same.
Why can two labs report different compositions for the same fabric?
Two competent labs can disagree because they are answering slightly different questions, usually on basis, pre-treatment or specimen choice.
| Cause of the gap | What differs | How to close it |
|---|---|---|
| Reporting basis | Clean dry mass against moisture allowances, or different allowance values | Write the basis and figures into the order |
| Pre-treatment | How much finish or size is removed first | Ask both labs to record the pre-treatment |
| Specimen location | One edge, one roll, or an incomplete pattern repeat | Specify lot, roll and full repeat |
| Method | ISO and AATCC routes are separate | Require one named method |
Compare the two report headers line by line first. If method and basis differ, you have two different measurements, not a disagreement.
How do moisture, finishes and sampling change the result?
Moisture regain is the mass of water a fibre holds, expressed as a percentage of its dry mass. Cotton holds far more than polyester, so adding allowances raises the cotton share on paper without changing a single fibre. EU Regulation 1007/2011 makes this explicit: results start on clean dry mass, then take agreed allowances. Elsewhere, values come from local rules or agreement.
Here is the same cloth, 65/35 on a clean dry basis, reported three ways. The allowances are the Annex IX values in that regulation: 1.5% for polyester, 8.5% for normal cotton and 10.5% for mercerised cotton.
| Reporting basis | Calculation | Polyester / cotton |
|---|---|---|
| Clean dry mass | 65 and 35 | 65.0 / 35.0 |
| With normal cotton allowance | 65 × 1.015 = 65.975; 35 × 1.085 = 37.975; total 103.95 | 63.5 / 36.5 |
| With mercerised cotton allowance | 65 × 1.015 = 65.975; 35 × 1.105 = 38.675; total 104.65 | 63.0 / 37.0 |
That is a 2-point move with no change to the fabric.
Finishes and size work the same way. Non-fibrous matter such as finishing oil or warp size adds mass that is not fibre, and ISO 1833-11 applies after its removal, so incomplete removal skews the result. In an illustrative case, a 65/35 cloth carrying 3% extra finish that goes into solution with the cotton reads 65 ÷ 103 = 63.1% polyester, with the remainder booked as cotton. Test at the stage you are buying, and say which stage that is.
Sampling decides what the number represents. A yarn-dyed check or dobby stripe must include a full repeat, or the ratio shifts with where the cutter landed. Blend ratios can also move between yarn lots, so a report from an earlier lot says little about yours. Treat it as evidence for that lot only, one of the checks when you verify a fabric supplier.
Who sets the composition tolerance, and how is it agreed?
A composition tolerance is the band around the declared ratio inside which the fabric still passes. Commercially it is set by agreement between buyer and supplier, per programme. Labelling law in your market can add its own rules, so confirm those separately.
Set the band from data:
- Test the approved sample twice, or at two labs, using the same method and basis.
- Note the gap. If repeats read 64.2 and 65.1, a band narrower than that 0.9-point gap can fail good cloth on noise alone (illustrative figures).
- Widen the band only as far as the end use allows. A 60/40 workwear twill depends on polyester for abrasion life, so downward drift matters.
- Set the action for a failure in advance: retest, referee lab, downgrade or reject.
A tighter band gives a stronger claim but more disputed lots. A wider one gives fewer disputes but a looser promise on the label.
On greige orders we coordinate, Burhan invoices per metre and sets the moisture regain convention per customer requirement. That is the invoicing side, covered in the metres vs kilograms guide, so write your composition basis into the order separately.
How should a composition clause be written into an order?
Copy these lines and fill in the blanks:
- Declared composition: 65% polyester / 35% cotton by mass, fibres named, not "65/35"
- Fibre identification: completed before quantitative analysis
- Method: ISO 1833-11:2017, or another named method
- Reporting basis: clean dry mass, or allowances of __% polyester and __% cotton (normal or mercerised)
- Tested stage: finished fabric, or loom state after size removal
- Sampling: __ specimens per lot, from named rolls, including a full pattern repeat
- Tolerance: ± __ percentage points per fibre, agreed for this programme
- Report must show: method, pre-treatment, basis, lot and roll reference
- Disagreement: named referee lab, retained sample from the same roll
Fit it alongside shrinkage, fastness and strength using this wider pre-bulk test list.
Burhan Enterprises is a sourcing partner in Karachi, not a mill: we match a requirement to suitable partner units and hold the specification and approvals through production. Send your clause with the enquiry through our Pakistan fabric supplier page.
Quick answers
How does a fabric composition test work? A fabric composition test identifies the fibres, then dissolves one with a selective reagent and weighs the dried residue. For polyester-cotton, sulphuric acid removes the cellulose and the polyester remains. The polyester share is residue dry mass divided by specimen dry mass, and the cotton share is found by difference.
Can a burn test prove a fabric is 65/35 polyester-cotton? No. A burn test can suggest that a synthetic fibre is present, because polyester melts into a hard bead while cotton chars to soft ash, but it gives no mass ratio. A contract claim of 65/35 needs quantitative fibre analysis under a named method, reported on a stated basis.
Why does a fabric test as 63.5/36.5 when the spec says 65/35? The reporting basis may have changed rather than the fabric. A cloth that is 65/35 on clean dry mass reads about 63.5/36.5 once moisture allowances of 1.5% for polyester and 8.5% for normal cotton are applied. Check the method and basis on both reports before raising a claim.
What composition tolerance should a buyer agree? Agree it per programme, because no single commercial figure fits every fabric. Test the approved sample twice under the same method and basis, then set a band wider than the gap between those repeats so that good cloth does not fail on noise. Keep it within what the end use and label claim allow.
Klaar om dit te sourcen?
Gratis stalen, eerlijke levertijden, één aanspreekbare partner.
Vraag gratis stalen aan