Streaks, Barré and Shade Bars: Is the Fault in the Greige or the Dyeing?
What causes streaks in dyed fabric? Trace barré, shade bars and stripes to the yarn, the loom or the dyehouse, confirm each, and keep the evidence for a claim.

Streaks in dyed fabric have two broad causes: differences already in the greige, such as yarn lot mixing, tension or pick-density variation and starting marks, or uneven preparation, dyeing or finishing. Direction, repeat interval, unravelled yarns and a stripped sample usually show which. Keep the roll uncut and record the evidence before raising a claim.
What causes streaks in dyed fabric?
A streak is any line or band of different shade that the design did not call for. Dye reveals differences in yarn and structure that are hard to see in loom-state cloth, so the stage where a fault shows is often not where it began.
| Fault | What it looks like | Likely origin | How to confirm | Evidence to keep |
|---|---|---|---|---|
| Barré or weft bars | Repeating bands across the width | Yarn lot mixing; weaving or knitting tension | Measure the repeat; compare unravelled yarns | Repeat in cm; yarn lot record |
| Warp streak | Line along the length, following set ends | Warp yarn mixing; warp tension | Trace it to specific ends; unravel them | Position across the width; warp lot |
| Pick bar (shade bar) | Sharp-edged band across the width | Pick-density variation | Count picks per inch in and out of the band | Both counts; metre position |
| Starting mark | Narrow full-width line, irregular spacing | Loom stop and restart | Count picks either side; check the greige | Metre position of each mark |
| Preparation streak | Cloudy, soft-edged lines or patches | Residual size; uneven scour or bleach | Crosses yarns; yarns match; glow under UV light suggests oil | Preparation route; photos |
| Rope or crease mark | Wandering lines along the length, no repeat | Rope-form dyeing; creases set in the machine | Follows folds, not yarns | Dye lot; machine type |
| Listing or ending | Drift from selvedge to centre, or roll start to end | Pad pressure; dye liquor change in the run | Compare side, centre, side and both roll ends | Colour readings by position |
| Finishing bar | Straight full-width band, often a single one | Stenter or pad stop; uneven finish pick-up | No yarn or pick difference across the band | Metre position; finishing lot |
How do you tell barré from a dyeing streak?
Barré is an unintended, repeating pattern of bars, usually parallel to the weft in woven cloth or to the courses in circular knit. Sources use the word inconsistently: some keep it for knits and call the woven version weft bars or shade bars. Describe the fault in writing by direction and repeat.
- Does it follow the yarns? A barré band starts and stops on specific picks or courses. A dyeing streak usually has soft edges, crosses yarns or follows a fold line.
- Does it repeat? A regular repeat points to a machine or yarn cycle. In circular knit, a repeat matching the feeder count, or a multiple of it, points to a single feeder or yarn package. In weaving, irregular spacing points to loom stops.
Sharp edges along yarns send you to the greige first, and soft edges that ignore yarns send you to the dyehouse first. Warp-wise lines need care, because a warp streak holds to the same ends while a rope mark wanders across them.
A flat, plain surface in a solid colour generally shows a bar more readily than a twill or a print. Very dark shades such as navy or black, and very light ones, can mask the colour difference.
Which faults start in the greige and survive dyeing?
Greige-origin faults sit in the yarn or the structure, so preparation does not remove them.
- Yarn lot mixing. Yarns from different spinning lots can differ in count, twist and fibre maturity, and take dye differently. The difference can be nearly invisible in loom state.
- Pick-density variation. On a 40 × 40 / 120 × 60 plain weave, a band at 57 picks per inch instead of 60 carries 5% less weft (3 ÷ 60). The cloth is more open there and reads as a different shade.
- Starting marks. After a loom stop, the first picks can beat up at a different density, leaving a line that often surfaces only after dyeing.
Header matching is the default greige inspection on Burhan-coordinated orders: a header, meaning a full-width cutting, is taken from every roll in the lot, the headers are matched against each other, and each is checked against the approved sample, with roll bodies inspected on a sampled basis. Our guide to pre-shipment greige inspection sets out the procedure.
A header shows a roll at one point and in loom state, so a latent dye-affinity difference may not show in it. For a solid colour, ask whether headers from suspect rolls can be trial-dyed before bulk. Differences between whole rolls or lots, rather than bands inside a roll, are a batch and shade continuity question.
Which faults come from preparation, dyeing or finishing?
Process faults ignore yarn boundaries, and yarns unravelled from inside and outside the mark usually match in thickness and twist.
Preparation. Dye lands unevenly where size, waxes or oils remain, giving cloudy, soft-edged shade variation. See what sizing and preparation remove.
Dyeing. Jet and winch machines run cloth in rope form, so lines can set where it folds. Open-width routes avoid rope marks but carry a risk of listing, when pad pressure or liquor differs across the width, and ending, when shade drifts from the start of a run to the end.
Finishing. A stoppage on a stenter or pad can leave a straight, full-width band where the cloth sat in heat or liquor.
How can a fault's origin be confirmed before a claim?
- Read direction and repeat. Unroll several metres, mark the warp direction and measure the distance between marks. This needs no cutting.
- Count density. Use a pick glass to count picks or ends per inch inside and outside the band.
- Unravel yarns. Compare thickness, twist and lustre of yarns from the band and from clean cloth beside it, across at least two repeats. A yarn difference points upstream of dyeing.
- Strip a sample. A lab or dyehouse removes the colour with chemistry suited to the dye class, then re-dyes it. If the band returns in the same place, that points to the substrate. If it does not, suspect dye application.
Stripping has limits. It is rarely complete, some dyes resist it, and a recurring band can still mean damaged preparation rather than bad greige. A useful comparison, if one was kept, is a greige header from the same roll, prepared and dyed in a lab, though it speaks only for that point in the roll. Treat all of this as strong indication rather than proof.
Testing needs fabric, and cutting can end a claim, so agree in writing who takes any sample and from where before anyone touches the roll.
What evidence should you keep, and when must you raise a claim?
Assemble this file as soon as a fault appears:
- Roll number, lot number, dye lot and the metre position of each mark
- Photos in consistent light, with a tape showing the repeat and an arrow showing warp direction
- Pick counts, repeat measurements and any lab report
- The approved sample, the order confirmation, the delivery date and the date you found the fault
On Burhan-coordinated greige orders, a valid claim is settled by 100% refund, raised within 15 days of delivery, on fabric uncut from the roll. Once a roll is cut there is no claim, so inspect on arrival. For other orders, read your order confirmation. Our buyer assurance page sets out how a claim is raised.
If you buy greige and dye it elsewhere, the 15 days still run from delivery of the greige, not from the day streaks appear. That is the practical case for trial-dyeing early.
To shorten a later dispute, put these on the order:
- Approved sample reference and inspection method
- Whether warp and weft can each come from one spinning lot
- Who takes test samples, and how a sample affects the claim
Burhan Enterprises is a Karachi sourcing partner, not a mill: we coordinate partner units and hold the specification and approvals through production. If you want a base you can inspect before committing colour, see low-MOQ greige cotton sourcing.
Quick answers
What causes streaks in dyed fabric? Greige causes include yarn lot mixing, tension or pick-density variation and starting marks. Processing causes include residual size, uneven scouring or bleaching, rope marks in jet dyeing, pad pressure differences and stenter stoppages. Direction, repeat interval and whether the mark follows individual yarns usually separate the two groups.
Is barré a yarn fault or a dyeing fault? Barré usually starts before dyeing, in yarn lot mixing or in tension and density differences during weaving or knitting. Dyeing reveals it rather than creates it, and the bands run parallel to the weft or courses and start and stop on specific yarns. Soft-edged marks that cross yarns point to the dyehouse instead.
How long do you have to raise a claim on a Burhan-coordinated greige order? A valid claim on a Burhan-coordinated greige order is settled by 100% refund, raised within 15 days of delivery, on fabric uncut from the roll. Once a roll is cut there is no claim. Inspect on arrival and raise the issue before any roll reaches the cutting table.
Which shades hide barré? Very dark shades such as navy or black, and very light shades, can mask the colour differences behind barré. Shades between those extremes leave it more visible, so a bar that looks minor in one colour may be obvious in another.
Prêt à sourcer ce tissu ?
Échantillons gratuits, délais honnêtes, un partenaire unique et responsable.