RFD Fabric Testing: Checking a Base Before It Goes to the Dyer

RFD fabric testing before dyeing: the absorbency drop test, residual size, whiteness and pH checks that catch a poor base, and how to write them onto an order.

RFD Fabric Testing: Checking a Base Before It Goes to the Dyer — article cover image

RFD fabric testing means checking a ready-for-dyeing base before colour goes on: an absorbency drop test, a residual-size spot test, a whiteness reading, a pH check on the water extract and a visual fault inspection. Dyeing cannot repair poor preparation, so test every lot and write the acceptance limits onto the purchase order.

Why does RFD fabric need testing before it is dyed?

RFD (ready for dyeing) is fabric that has been desized, scoured and usually bleached so that it takes colour evenly. The RFD fabric definition covers what the term promises and what it leaves open. "RFD" describes a processing state, not a measured result. Two suppliers can both call a lot RFD while one has left wax in the selvedges and size in the warp.

Faults are quick to find in white cloth and costly to fix in coloured cloth. A slow-absorbing zone takes minutes to detect on a white roll. Once dyed, it becomes a patchy shade across a full dye lot, which usually ends in stripping and re-dyeing or a shade downgrade. Readings taken before dispatch also help settle the usual dispute over whether the base or the dyeing failed.

How does the absorbency drop test work, and what does a slow drop mean?

The absorbency drop test times how long one drop of water takes to soak into the fabric. The reference method is AATCC TM79, Test Method for Absorbency of Textiles: a drop falls from a fixed height onto taut fabric, and the operator records the seconds until the drop stops reflecting light. Well-prepared cotton typically absorbs a drop in a few seconds. Loom-state greige can hold a bead for a minute or more.

A slow drop usually has one of three causes:

  • Incomplete scouring: natural waxes and pectins remain, so the cloth repels water.
  • Residual size: a film left on the warp yarns keeps water off the fibre.
  • An unwanted finish: a softener or silicone added to improve the hand of the base.

The spread matters more than the average. Test edge, centre and edge across the width, at the start, middle and end of the roll. A roll that averages fast but stalls near one selvedge can dye lighter or darker on that side, a fault called listing. On warp-faced twills and drills, test both faces: the size sits on the warp yarns, and the two faces can read differently.

The limit belongs to the dyer, since dye routes tolerate different absorbency: agree a maximum in seconds per programme.

How do you check whether size has really been removed?

Residual size is the starch, PVA or acrylic film applied to the warp before weaving that preparation failed to strip. The guide to sizing and preparation explains why it must come out first. Starch is checked with an iodine spot test: iodine solution turns blue-black to violet where starch remains, and the colour is graded on a 1 to 9 violet scale, commonly called the TEGEWA scale, where 9 means no starch is left. PVA does not show reliably with plain iodine, so an iodine and boric acid reagent is used instead, turning blue where PVA remains. Starch turns it blue too, so run plain iodine first.

Ask the weaver what the warp was sized with before choosing the test: a starch test on a PVA-sized warp passes a dirty base, and an acrylic-sized warp needs its desizing route confirmed with the processor. Then spot-test near the selvedges and along any crease, where size survives longest.

Do whiteness and pH matter on an RFD base?

Yes, depending on the shade. Whiteness is how white the base reads to a standard observer, measured on a spectrophotometer as a CIE whiteness value; AATCC TM110, Test Method for Whiteness of Textiles, is the common reference. CIE values are relative, so compare the lot against a retained reference on the same instrument, not a figure from another lab.

For pastels and digital prints, whiteness drives the result: a creamy base pulls every pale colour towards yellow. For navy, black and deep reds, a half-bleached base is often acceptable and gentler on fibre strength. State whether optical brightener is allowed. Brightener can shift a pale shade under light with ultraviolet content, so bases intended for colour are commonly specified without it.

pH is measured on a water extract of the fabric, per AATCC TM81, Test Method for pH of the Water-Extract from Wet Processed Textiles. A high reading usually means alkali from scouring or bleaching was not washed out. Leftover hydrogen peroxide from bleaching is a separate risk, checked with a peroxide test strip. Either interferes with dye chemistry, reactive dyes especially, and shows as shade drift between batches. Agree a near-neutral band with the dyer.

What does each RFD fault look like once the fabric is dyed?

Fault in the RFD baseHow to catch it before dyeingWhat it looks like after dyeing
Slow or uneven absorbencyDrop test across width and lengthPatchy, cloudy shade; side-to-centre variation
Residual sizeIodine or iodine-boric acid spot testPale streaks along the warp, stiff hand, weak rubbing fastness
Residual alkali or peroxideWater-extract pH, peroxide stripShade off target, drift between batches, duller colour
Low or uneven whitenessCIE whiteness against a retained referenceDull or yellowed pale shades
Optical brightener presentAsk, then check under a UV lampPale shade that changes between light sources
Motes and seed-coat specksVisual check on a lit tableDark specks in pale shades
Crease or rope marksVisual check, full widthLight or dark lines that do not press out
Pinholes or weakened fibreVisual check; tear strength against agreed minimumHoles after finishing, seams that tear
Oil or grease stainsVisual checkResist spots, usually lighter than the ground

Weak fastness is the fault that hides longest. When size or wax sits between dye and fibre, colour builds on the surface instead of penetrating, so the cloth can match on the table and then fail rubbing or washing tests at garment stage. Approve the lab dip on cloth from the actual RFD lot, not the dyer's stock base.

What acceptance lines should an RFD purchase order carry?

Write each limit as a number, a method and a sampling plan. Leave each figure blank until the dyer states it.

  • Base: [composition], [construction], [GSM ± agreed], [finished width], prepared for [reactive dyeing / vat dyeing / rotary print / digital print].
  • Absorbency: AATCC TM79 drop test at 3 points across the width, at start, middle and end of each sampled roll; every reading ≤ [x] seconds.
  • Residual size: size type declared by the weaver; iodine (starch) or iodine and boric acid (PVA) spot test; starch rated ≥ [x] on the violet scale, no PVA colour.
  • Whiteness: CIE whiteness per AATCC TM110 ≥ [x] against the retained reference, same instrument; optical brightener: none.
  • pH: water extract per AATCC TM81 within [x to y]; residual peroxide: nil on test strip.
  • Visual: no motes visible at [distance], no crease or rope marks, no holes, no oil stains.
  • Sampling: [every roll / x rolls per lot]; results reported before dispatch to the dyer.
  • Approval: lab dip or dyed test swatch from this lot, in the target shade, before bulk dyeing.
  • Non-conforming rolls: held and not dyed until resolved.

Before buying a prepared base at all, the greige vs RFD comparison shows what preparation adds.

Burhan Enterprises is a sourcing partner in Karachi, not a mill: we match a requirement to suitable partner units and hold the specification and approvals through production. For prepared bases by composition and route, see RFD fabric sourcing.

Quick answers

What is RFD fabric testing? RFD fabric testing is the set of checks a ready-for-dyeing base should pass before colour is applied: absorbency by water-drop test, a residual-size spot test, CIE whiteness, pH of the water extract and a visual inspection for motes, creases, holes and stains. Dyeing reveals preparation faults but cannot repair them.

How fast should an RFD fabric absorb a drop of water? There is no universal figure, so the limit should come from the dyer for each programme. Well-prepared cotton typically absorbs a drop in a few seconds, while loom-state greige can hold a bead for a minute or more. Consistency matters as much as speed, because one slow zone near a selvedge is enough to cause side-to-centre shade variation.

Which test shows whether size is still on an RFD base? Starch size is detected with an iodine spot test, which turns blue-black to violet where starch remains and is graded on a 1 to 9 violet scale, with 9 meaning none left. PVA size needs an iodine and boric acid reagent, which turns blue; starch does too, so test for starch first. Ask the weaver what the warp was sized with first, because the wrong test can pass a dirty base.

Should an RFD base contain optical brightener? A base intended for dyeing is commonly specified without optical brightener. Brightener makes white cloth look whiter by fluorescing under ultraviolet light, which can make a pale dyed shade change between light sources. An optic-white finished fabric is a different specification, so the purchase order should state which one is being bought.

Prêt à sourcer ce tissu ?

Échantillons gratuits, délais honnêtes, un partenaire unique et responsable.

Demander des échantillons gratuits

Notes sourcing par e-mail

En vous abonnant, vous acceptez de recevoir nos analyses sourcing par e-mail. Désinscription possible à tout moment. Voir notre politique de confidentialité.

Un besoin en tissu ?

Dites-nous ce que vous fabriquez — nous vous aiderons à le sourcer.

Demander des échantillonsWhatsApp